Polysulfone

Chemical rating key:
A = Little to no Interaction
B = Slight Interaction
C = Not Recommended

Polysulfone
Chemical Rating Notes
Acetic acid, 10%
A
Acetic acid, 20%
A
Acetic acid, 50%
B
Elevated temperatures may reduce resistance.
Acetic acid, glacial
A
Elevated temperatures may reduce resistance.
Acetic anhydride
C
Acetone, 5%
A
Acetone, 50%
A
Acetone, 60%
A
Exposure to elevated stress may damage polymer.
Acetonitrile
C
Acetophenone
C
Acetyl choride
C
Adhesive (Eastman 910)
A
Aluminum sulfate, 10%
A
Aluminum Trichloride, 10%
A
Aminoethanol (2-)
A
Ammonia, 29%
A
Exposure to elevated stress may damage polymer.
Ammonium chloride, 10%
A
Ammonium hydroxide, 15%
A
Elevated temperatures may reduce resistance.
Ammonium hydroxide, 29%
A
Elevated temperatures may reduce resistance.
Ammonium nitrate, 10%
A
Ammonium persulfate, 24%
A
Ammonium sulfate, 10%
A
Amyl acetate
C
Amyl alchohol
A
Aniline
C
Anti-Freeze
A
Exposure to elevated stress may damage polymer.
Antimony trichloride, saturated
C
Automotive grease
A
Exposure to elevated stress may damage polymer.
Aviation gasoline (100 octane)
B
Prolonged Exposure May Reduce Resistance
Barbitol solvent
A
Barium chloride, 10%
A
Benzaldehyde
C
Benzene
C
Benzene sulfonic acid
C
Benzonitrile
C
Benzyl chloride
C
Black liquor
A
Elevated temperatures may reduce resistance.
Brake fluid
C
Bromine, 10%
B
Butanol
A
Exposure to elevated stress may damage polymer.
Butter, salted
A
Exposure to elevated stress may damage polymer.
Butyl acetate
C
Butyl alcohol
A
Butyl cellosolve
A
Butyl ether
A
Butyl phthalate
C
Butylamine (n-)
C
Butylated hydroxy anisole
C
Butylated hydroxy toluene
A
Calcium chloride, saturated
A
Calcium Dinitrate, 10%
A
Calcium hypochlorite, 3.5%
A
Prolonged Exposure May Reduce Resistance
Calcium propionate
A
Exposure to elevated stress may damage polymer.
Calgon liquid
A
Carbitol
A
Carbon tetrachloride
A
Prolonged Exposure May Reduce Resistance
Cellosolve (2-ethoxyethanol)
A
Cellosolve solvent
A
Room temperature only.
Chlorine
C
Chlorine, wet
C
Chlorobenzene
C
Chloroethanol (2-)
C
Chloroform
C
Chlorophenol, 5%
C
Chromic acid, 10%
A
Chromic acid, 12%
A
Exposure to elevated stress may damage polymer.
Chromic acid, 60%
C
Citric acid, 40%
A
Corn oil
A
Exposure to elevated stress may damage polymer.
Cotton Seed oil
A
Exposure to elevated stress may damage polymer.
Cresol (m-)
C
Cresyldiphenyl phosphate
C
Cupric chloride, saturated
A
Cyclohexane
A
Exposure to elevated stress may damage polymer.
Cyclohexanol
A
Cyclohexanone
C
Dichlorobenzene (p-), vapor
C
Dichlorodifluoromethane (Freon 12)
A
Diesel fuel
A
Diesel fuel (fuel oil #2)
A
Diethylene glycol
C
Dimethyl sulfoxide
C
Dimethylaniline
C
Dimethylformamide (N,N-)
C
Dioctylphthalate
A
Exposure to elevated stress may damage polymer.
Dioxane (p-)
C
Dowtherm
C
Epichlorohydrin
C
Ethanol
A
Exposure to elevated stress may damage polymer.
Ether
C
Ethyl acetate
C
Ethylbutyric acid (2-)
A
Ethylene chloride
C
Ethylene glycol
A
Ethylenediamine, 92%
A
Room temperature only.
Ferric chloride, 10%
A
Ferrous sulfate, saturated
A
Formaldehyde, 37%
A
Elevated temperatures may reduce resistance.
Formic acid, 10%
A
Formic acid, 88%
C
Freon 11
A
Elevated temperatures may reduce resistance.
Freon TMC
C
Freon TMS
A
Exposure to elevated stress may damage polymer.
Furfural
C
Gasoline
A
Exposure to elevated stress may damage polymer.
Glycerin
A
Grape juice
A
Grease
A
Exposure to elevated stress may damage polymer.
Green liquor
A
Heptane (n-)
A
Exposure to elevated stress may damage polymer.
Heptane, .05%
A
Hexane (n-)
B
Exposure to elevated stress may damage polymer.
Hydraulic oil
A
Hydrobromic acid, 20%
A
Hydrochloric acid, 20%
A
Exposure to elevated stress may damage polymer.
Hydrochloric acid, 37%
A
Elevated temperatures may reduce resistance.
Hydrofluoric acid, 50%
A
Prolonged Exposure May Reduce Resistance
Hydrogen peroxide
A
Isooctane
A
Isopropanol
A
Prolonged Exposure May Reduce Resistance
Isopropyl ether
B
Prolonged Exposure May Reduce Resistance
Jet fuel (JP-4)
A
Jubilee wax
A
Room temperature only.
Kerosene
A
Exposure to elevated stress may damage polymer.
Ketchup
A
Lactic acid, 60%
A
Prolonged Exposure May Reduce Resistance
Lard
A
Lauric acid
A
Prolonged Exposure May Reduce Resistance
Lemon oil
C
Lestoll
C
Linseed oil
A
Lubricating oil
A
Magnesium chloride, 10%
A
Malonic acid
A
Margarine
A
Exposure to elevated stress may damage polymer.
Mayonnaise
A
MEK, 40%
A
Exposure to elevated stress may damage polymer.
Methanol
A
Exposure to elevated stress may damage polymer.
Methylene chloride
C
Milk
A
Exposure to elevated stress may damage polymer.
Mineral oil
A
Monochlorodifluoromethane (Freon 22)
B
Prolonged Exposure May Reduce Resistance
Monoethanolamine
A
Morpholine, .2%
C
Motor oil
A
Mustard
A
Naphtha VMOP
C
Naphthalene, vapor
C
Nitric acid, 10%
A
Nitric acid, 20%
A
Room temperature only.
Nitric acid, 40%
A
Room temperature only.
Nitric acid, 5%
A
Exposure to elevated stress may damage polymer.
Nitric acid, 71%
C
Nitro Methane
C
Nitrobenzene
C
Oil (ASTM #1)
A
Oil (ASTM #2)
A
Oil (ASTM #3)
A
Exposure to elevated stress may damage polymer.
Oleic acid
A
Exposure to elevated stress may damage polymer.
Olive oil
A
Prolonged Exposure May Reduce Resistance
Oxalic acid, 20%
A
Oxygen
A
Ozone
A
Peanut oil
A
Exposure to elevated stress may damage polymer.
Permatex
A
Exposure to elevated stress may damage polymer.
Phenol
C
Phosphoric acid, 20%
A
Phosphoric acid, 85%
A
Photographic film developer
A
Photographic film fixer
A
Potassium hydroxide, 20%
A
Potassium hydroxide, 35%
A
Potassium nitrate, saturated
A
Potassium permanganate, 10%
A
Pyridine
C
Silastic 140
A
Silicone compounds
A
Exposure to elevated stress may damage polymer.
Sodium bicarbonate, 10%
A
Sodium carbonate, 10%
A
Sodium chloride, 10%
A
Sodium chromate, 10%
A
Sodium hydroxide, 15%
A
Sodium hydroxide, 25%
A
Elevated temperatures may reduce resistance.
Sodium hydroxide, 30%
A
Elevated temperatures may reduce resistance.
Sodium hydroxide, 5%
A
Sodium hydroxide, 50%
A
Elevated temperatures may reduce resistance.
Sodium hypochloride, 10%
A
Sodium hypochlorite, 0.17%
A
Sodium silicate, 1.7%
A
Exposure to elevated stress may damage polymer.
Sodium sulfate, 10%
A
Sodium sulfide, 10%
A
Sodium thiosulfite, 10%
A
Sorbic acid
A
Stoddard Solvent
A
Exposure to elevated stress may damage polymer.
Sulfolane
C
Sulfuric acid, 30%
A
Prolonged Exposure May Reduce Resistance
Sulfuric acid, 5%
A
Prolonged Exposure May Reduce Resistance
Sulfuric acid, 65%
A
Prolonged Exposure May Reduce Resistance
Sulfuric acid, 85%
A
Prolonged Exposure May Reduce Resistance
Sulfuric acid, 95%
C
Surfactant (Jet-Dry)
A
Tetrachlorodifluoroethane (Freon BF)
A
Exposure to elevated stress may damage polymer.
Tetrahydrofuran (THF)
C
Toluene
C
Toluene, 0.05%
B
Prolonged Exposure May Reduce Resistance
Tomato juice
A
Transmission oil
A
Trichloroethane (1,1,1-)
B
Exposure to elevated stress may damage polymer.
Trichloroethylene
C
Trichlorofluoroethane (Freon TF)
A
Triphenylphosphite
C
Turpentine
C
Varsol
A
Exposure to elevated stress may damage polymer.
Vegetable oil
A
Exposure to elevated stress may damage polymer.
Water
A
Xylene
C
Zinc chloride, saturated
A